This study investigated the effect of flux type and amounts on recovery behavior of aluminum alloy during the melting process of Al can scrap. The heat treatment was conducted to remove the coating layer on the surface of can scrap at 500°C for 30 min. The molten metal treatment of the scrap was performed at 750°C in a high-frequency induction furnace with different flux types and amounts. It was observed that the optimum condition for recovery of Al alloy was to add about 3 wt.% flux with a salt and MgCl2 mixing ratio of 70:30 during melting process. The mechanical properties of recovered Al alloy were about 254.8 mPa, which is similar to that of the virgin Al5083 alloy.