Effect of carbon content on the fracture toughness of Ni-Cr-Mo steels

Wybrane pełne teksty z tego czasopisma
Identyfikatory
Warianty tytułu
PL
Wpływ węgla na odporność na pękanie stali Ni-Cr-Mo
Języki publikacji
EN
Abstrakty
EN
In this paper the effect of carbon content on the fracture toughness changes with tempering temperaturę of three Ni-Cr-Mo steels containing so-called strong „background" of other alloying elements is presented. The effect of tempering temperaturę on the steels' toughness was examined by the linear elastic fracture mechanics (KIc test). It was demonstrated that alloys containing 0.10 and 0.31% C are characterized by high fracture toughness and Iow ability to irreversible embrittlement after Iow - temperaturę tempering. The alloy containing 0.79% C is characterized by the lowest fracture toughness within the whole rangę of tempering temperaturę. Mechanical investigations were also supplemented with fracture surfaces observations. The obtained results are supposed to complement the existing software and d-bases pertaining to the quantitative effect of elements on steels' properties.
PL
W pracy przedstawiono wyniki badań wpływu węgla na zmiany odporności na pękanie z temperaturą odpuszczania trzech stopów modelowych stali Ni-Cr-Mo zawierających tzw. silne „tło" innych pierwiastków stopowych. Zmiany odporności na pękanie stopów z temperaturą odpuszczania określono metodą liniowo - sprężystej mechaniki pękania (przez pomiar współczynnika intensywności naprężeń KIc). Wykazano, że stopy zawierające 0,10 i 0,31% C charakteryzują się bardzo dobrą odpornością na pękanie i małą wrażliwością na kruchość odpuszczania I rodzaju po niskim odpuszczaniu. Najmniejszą odpornością na pękanie w całym zakresie temperatur odpuszczania cechuje się stop zawierający 0,79% C. Badania mechaniczne dodatkowo poparto dokumentacją fraktograficzną przełomów próbek. Wyniki badań uzyskane w niniejszej pracy z pewnością uzupełnią istniejące już programy komputerowe oraz bazy danych dotyczące ilościowego wpływu pierwiastków stopowych na własności stali.
Twórcy
autor
autor
  • AGH University of Science and Technology, Al. Mickiewicza 30, 30-059 Kraków
Bibliografia
  • [1] R. W. K. Honeycombe, H. K. D. H. Bhadeshia, Steels. Microstructure and properties, 2nd ed. London: Edward Arnold (1995).
  • [2] A. K. Sinha, Physical Metallurgy Handbook, The Mc Graw-Hill Companies, Inc. (2003).
  • [3] J. Pacyna, B. Pawłowski, The effect of the tem-pering temperature on 30HGSNA steel toughness, Metallurgy and Foundry 10, 4, 409-421 (1984).
  • [4] A. Jędrzejewska-Strach, Manganium influence upon the kinetics of phase transformations, struc-ture and ąualities of model construction steel alloys, Ph.D. Thesis, AGH University of Science and Technology, Kraków, 1995.
  • [5] M. Dubiel, Phase transformation in model alloys with chromium imitating the matrix of quenched construction and rustless steels, Ph.D. Thesis, AGH University of Science and Technology, Kraków, 1996.
  • [6] M. Strach, The structure and ąualities of silicon steels evaluated on the basis research of model alloys of vari-ous silicon and carbon concentration, Ph.D. Thesis, AGH University of Science and Technology, Kraków, 1995.
  • [7] R. Dąbrowski, The effect of vanadium on the structure and properties of ąuenched and tempered model alloy steels, Ph.D. Thesis, AGH University of Science and Technology, Kraków, 2002.
  • [8] R. Dąbrowski, J. Pacyna, J. Krawczyk, New high hardness Mn-Cr-Mo-V steel, Archives of Metallurgy and Materials 52, 1, 87-92 (2007).
  • [9] G. Zając, The structure and properties of ąuenched and tempered steels with nickel, Ph.D. Thesis, AGH Univer-sity of Science and Technology, Kraków, 2006.
  • [10] A. P. Gulyaev, The fracture work decomposition in impact resistance test on the components on the ground of impact resistance test samples with different notches, Zavodskaja Laboratoria 33, 4, 473-475 (1967), (in Russian).